Property type: Hotel
Location: Atlanta, GA
Client: Attorney for plaintiff (family of the deceased)
Case Summary:
Lashawna Threatt, a 30-year-old Atlanta model and mother, was hosting a small birthday party in her 10th-floor hotel room. Friends remember her as warm, affectionate, and “all love.” She and a friend were crouching near the floor-to-ceiling windows and leaning against the glass when it suddenly broke. Both women fell backward through the opening.

Lashawna landed on a skylight below and died of multiple blunt traumas. She was survived by her teenage daughter, her fiancé, and her family. Her friend rolled down the skylight, fell further to the sidewalk, and survived with permanent injuries.

The window glass measured about 45″ wide × 37″ tall × 0.190″ thick. The floor-level glass was neither tempered nor laminated, so it was not safety glass.
What Façade Consultants Reviewed
- Depositions of witnesses, the Property Manager, and the Building Engineer
- Construction documents and site photographs
- CPSC 16 CFR Part 1201, the federal Safety Standard for Architectural Glazing Materials
First Site Investigation: Signs of Poor Maintenance
The room’s entire exterior wall was a floor-to-ceiling window wall with a horizontal mullion 39.5″ above the floor. Three conditions stood out:
- Shrunken interior glazing gaskets. They had pulled back and were giving the glass little support.

The hotel windows and glass were found in a state of poor maintenance that weakened the glass. The glass was poorly supported and there was even a crack in one of the other panes of glass in the same room - “Cap beaded” exterior glazing. Glass edges had been caulked to the frame, and two layers of sealant suggested repeated attempts to fix a leak.

Dangerous, poorly supported glass contributed to the glass breakage and window fall. Evidence of previous repair attempts shows that a problem already existed (probably leakage). - A cracked pane in the same room. The crack was dirty, meaning it had gone unrepaired for years. Cracks weaken glass, which raised the question of whether the incident glass was also weakened by pre-existing damage.

Crack in adjacent hotel glass (at top) indicates surprisingly lax maintenance, giving rise to the suspicion that the incident glass (at bottom) was also weakened.
Second Site Investigation: Examining the Cracked Pane
Façade Consultants attended a forensic exercise in which the cracked glass, with its 3″ crack, was removed. The crack began at an edge chip left from original construction, decades before the incident.
Fragment Examination and Attempted Reassembly
To look for fractographic evidence of pre-existing damage, we built a full-size, scaled template of the recovered shards and tried to reassemble the broken window.

- We extended some crack edges and found three possible crack convergence points.

Meshulam assembles the incident glass shards in the search for more information on the glass breakage leading to the fatal fall - A tin-side detector identified which face of each shard was the “tin side” (the side floated on molten tin in the float glass process), so the shards could be placed in the correct up/down orientation.

Window glass has a “tin side” which is the side that was floated on a bed of molten tin during the float glass process. Here a detector is used to determine the tin side in order to assist in reassembling the glass puzzle - Every fragment was photographed and catalogued.

We could not positively locate the crack origin, but the effort was worth making.
Glass Impact Testing: When Does Glass Stop Being a Barrier?
Façade Consultants designed a test protocol to measure how well different glass types resist a human fall-through. We followed CPSC 16 CFR 1201 as closely as possible, using a 100 lb impactor swung or dropped against the glass.
The vertical drop height sets the impact energy. A 1-foot drop delivers 100 foot-lbs (100 lb × 1 ft). The federal standard uses only 18″ and 48″ drop heights (150 and 400 foot-lbs). We made two changes:

- We started at smaller drop heights and ramped up with repeated impacts.
- We evaluated breakage by the point at which the glass stopped acting as a barrier against a person falling through. We called this “break-through.”

How Each Glass Type Performed
Annealed glass breaks into large, dagger-like shards and clears the opening readily. It offers no resistance to a falling person and can cut them on the way out. This is why safety glass is required where human contact is likely.

Tempered glass was about twice as strong against blunt impact in our small study. It breaks into hundreds of small cubes that cut less severely than annealed shards, but the cubes easily leave the opening and provide no resistance to a fall.

Laminated glass (¼″ thick, two ¼″… see note) cracked readily under impact, but the pieces stayed bonded to the PVB (polyvinyl butyral) interlayer. It resisted fall-through better than any other glass type. Laminated and tempered glass are the two officially recognized safety glazing types.

Test Results
We tested glass taken from the hotel alongside new annealed, tempered, and laminated glass. Only one of the two panes removed from the building survived shipping to the lab.

- The hotel’s glass broke on the very first impact, at a 3″ drop height (25 foot-lbs).
- New annealed glass performed about six times better than the old hotel glass.
- Tempered and laminated glass performed far better at preventing a fall-through.

Why Did the Hotel Glass Break So Easily?
Glass weakens over time as it weathers. Glass engineers build a weathering factor into strength calculations that assumes about a 20-year life. The hotel’s glass was 37 years old at the time of the incident, nearly double that assumption. Many older buildings share this problem.
Building Code Compliance
- The glass met wind load requirements.
- It did not meet safety glazing requirements at original construction in 1973.
- It did not meet safety glazing requirements during a 2006 renovation, including the 2006 International Building Code.
- There was an ongoing history of glass breakage in the building in the years before the incident.
Façade Consultants’ Opinion
Ownership and management failed in their duty to provide a safe place for guests. They allowed the windows to remain in poor repair and failed to recognize or warn guests that the glass was weakened and breaking. Safety glass should have been used in the floor-level application. These failures were proximate causes of the death and injury.
Case Outcome
Monetary settlement. The hotel also committed to adding safety film to its floor-level glass.
Related Case Studies and Reading
- Similar incident: Glass façade shatters, woman dies after 25-foot fall from restaurant in Kolkata
- Another hotel glass breakage investigation
- Another hotel glass breakage investigation, with injury
Need a Glass Expert Witness?
If your case involves a window fall, glass breakage, or glazing failure, contact Façade Consultants to discuss how we can help.